Lightning  WC10Co4Cr HVOF coating leaves some lumps on the surface
Dear All

Lately we sprayed WC10Co4Cr using TAFA JP-5000 on paper industry rollers. We only have 2 sets of parameter which are 98g/min and 55g/min. Normally we would use 98g/min parameters with an actual feed rate of 70g/min. The thing is this time we use 98g/min parameter with an actual feed rate of 98g/min as well. After spraying and grinding, there were some metal lumps all over the roller's surface. Now we are looking at two main reasons.

1. We didn't dry off the powder by heat before using it.
2. We used too high feed rate even the Bulletin suggested so. And that caused unmelts parameters due to insufficient heat.

Please find pictures here

Also, find parameters that I mentioned as attached files.

Any reply would be useful. Thanks guys
Mad0233


Attached Files
.pdf   1350VM Tungsten Carbide-10% Co, 4% Cr (1.9.2.2SH-1350VM) (1).pdf (Size: 291.08 KB / Downloads: 128)
.pdf   1350VF Tungsten Carbide-10% Co, 4% Cr (1.9.2.2SH-1350VF).pdf (Size: 306.71 KB / Downloads: 116)
Reply
10-17-2023, 07:32 AM, (This post was last modified: 10-17-2023, 07:32 AM by Vadim Verlotski.)
#2
RE: WC10Co4Cr HVOF coating leaves some lumps on the surface
There are only two causes of lumps in thermal spraying, which are very clear and always the same:

1. Material first sticks to the inner surface of the nozzle and then periodically pops off this surface forming large particles (also known as "spitting").
2. Spray powder contains lumps that remain throughout the conveyance up to the nozzle.

Why does material stick to the inner surface of the nozzle? There are various reasons, but in your case the most obvious is: too much powder feeding.

The second cause of lump formation can also occur in your case: a powder that has been stored for a long time can collect moisture from the air and form lumps. Countermeasures include drying, keeping warm and sieving, which is why preheating the powder is important.
Reply




Possibly Related Threads…
Thread Author Replies Views Last Post
  Surface corrosion when HVOF spraying vcduramais 4 2,160 08-20-2021, 11:25 AM
Last Post: vcduramais
  surface speed for HVOF coating process gito 8 5,696 05-03-2019, 01:08 PM
Last Post: Lemster68
  WC10Co4Cr accumulation in JP5000 nozzle irishcorker61 1 2,149 04-06-2019, 08:26 AM
Last Post: Vadim Verlotski
  Coating for cyclone internal surface Arturas 0 1,922 12-11-2018, 06:58 AM
Last Post: Arturas
  Remove HVOF Coating in airfoil surface blade achmadarifudinh 5 3,923 07-20-2018, 10:51 AM
Last Post: achmadarifudinh
  Coating surface roughness William 9 26,781 12-26-2017, 10:40 AM
Last Post: Vadim Verlotski
  Powder Coating for Surface Table achmadarifudinh 3 3,808 11-28-2017, 12:19 PM
Last Post: Artyom
  Un-common surface pattern on coating failure shantanu 2 3,743 10-06-2016, 02:55 PM
Last Post: Vig
  Boron Carbide as a Surface Coating TCHP222 0 3,804 11-12-2015, 08:06 PM
Last Post: TCHP222
  Metco 450 coating surface problem Yaakov 2 6,787 05-06-2015, 01:54 PM
Last Post: loriolo
  HVOF coating over Induction Hardened surface shantanu 1 3,966 01-30-2015, 08:17 PM
Last Post: djewell
Rolleyes Discontinuities on HVOF surface Gabriel AM 3 4,908 05-29-2014, 08:22 PM
Last Post: KevinS
  Surface contact stress limit over an HVOF coating HVoilF 1 5,245 05-22-2013, 02:07 PM
Last Post: djewell
Question how can i find WC10Co4Cr propreties ? vladutzu86 0 3,002 02-03-2012, 04:02 PM
Last Post: vladutzu86
  Surface Speeds and traverse for coating Cro-167 js2know 2 7,016 12-23-2011, 02:15 PM
Last Post: Gordon



Users browsing this thread: 1 Guest(s)





Surface Engineering Forum Sponsor - Alphatek Hyperformance Coatings Ltd