HIPOJET 2700 PARAMETERS
09-11-2018, 06:07 PM,
#1
HIPOJET 2700 PARAMETERS
HELLO

Just acquired this HVOF unit
We mostly spray Tungsten and Chromium Carbides (fine mesh powders)

Would like to know what would be the OPTIMAL parameters to obtain the highest hardness and lowest porosity.

We use propane as Fuel.

Thanks in advance for the help.
Reply
09-17-2018, 07:57 PM,
#2
RE: HIPOJET 2700 PARAMETERS
Propane 60-65
6,2 Kgcm

Oxy 280-290
10.2 KGcm

Carrier gas 12
5 kgcm

Powder feeder 38 gr = 3 rpm

Spray distance 200 mm
Max surface temp 120
Preheat 90
Reply




Possibly Related Threads…
Thread Author Replies Views Last Post
  coating hardness using Hipojet 2700M air cooled JRB VIRANI 10 6,617 03-08-2020, 06:41 AM
Last Post: Stephen Booth
  parameter DJ GUN 2700 gito 0 2,546 03-26-2019, 03:28 AM
Last Post: gito
  SG-100 + ext. 2700 - spraying parameters Jaryn 1 3,598 11-27-2017, 02:21 PM
Last Post: Artyom
  DJ 2700 System Water cooled RV_DMG 3 6,108 03-14-2015, 05:05 AM
Last Post: Stephen Booth
  DJ 2700 nozzle for hydrogen RV_DMG 1 3,930 10-27-2014, 12:33 AM
Last Post: KevGarty
  DJ 2700 is oxygen temperature important? Thomas 3 5,808 11-01-2012, 10:16 AM
Last Post: davclark
  Powder fluidity and injector clogging (DJ 2700 HVOF gun). pulaunias 7 13,543 04-19-2010, 03:16 PM
Last Post: Gordon



Users browsing this thread: 1 Guest(s)





Surface Engineering Forum Sponsor - Alphatek Hyperformance Coatings Ltd