How to decrease interface contamination
02-23-2012, 09:35 AM,
#1
How to decrease interface contamination
hello friends,

I am troubled by sand blasting interface contamination these days.
We are doing HVOF coating on a landing gear axle (material is 300M,hardness is about 57HRC).
we sand blasted with the following parameters:
sand: F70 white alumina
Pressure:3.5-3.8bar
Nozzle diameter:5.8mm (two pressure gun)
angle:60
distance:200-250mm

The requirement is: check under ×200 microscope, in each field of view (not average), the interface contamination should lower than 10%.

I have tried many times, I even brushed the samples with nylon and copper brush, and then put it in the supersonic cleaning.
But in one or two field of view, we still can see some sand embed.

Have you ever sand blasting on this material?
Is it possible to achieve that criteria?
Reply
02-23-2012, 02:49 PM,
#2
RE: How to decrease interface contamination
Here are some thing you can do to reduce the interface contamination:
1, F70 is very fine grit for blasting, try to use bigger size.
2, 3.5-3.8 bar can be reduce to 2 bar.
3, How often do you change the grit? Maybe the blaster is too dirty.
Reply
02-24-2012, 07:04 AM,
#3
RE: How to decrease interface contamination
(02-23-2012, 02:49 PM)derek Wrote: Here are some thing you can do to reduce the interface contamination:
1, F70 is very fine grit for blasting, try to use bigger size.
2, 3.5-3.8 bar can be reduce to 2 bar.
3, How often do you change the grit? Maybe the blaster is too dirty.

Thank you Derek! I will try as you advised.
Our sand is recycled. After sand blasting, the sand will be seperated by screens. Some good size particles will be collected and recycled.

Reply




Possibly Related Threads…
Thread Author Replies Views Last Post
  Corrosion or Contamination on JP8000 xxxxmgulkokan 2 1,207 03-26-2022, 06:33 AM
Last Post: RAY SENFENG
Lightbulb Metco 58NS CuNiIn Interface Problem johnrafiee 18 5,071 03-15-2022, 07:57 AM
Last Post: techmankpo
  NiCrAlY interface separation edrazee 10 4,584 03-05-2020, 01:10 AM
Last Post: edrazee
  interface problem marzal 14 11,032 09-25-2015, 11:00 AM
Last Post: Joris Kraak
  Heat treatment after HVOF process to decrease porosity Giroud 3 6,291 07-13-2015, 05:51 AM
Last Post: aerotherm
  interface contamination Brent 5 8,393 04-06-2012, 06:04 PM
Last Post: Brent
  How to decrease the bigger voids of Ni-18.5Cr-6Al coating? Justin 3 4,488 12-17-2011, 03:41 AM
Last Post: Gordon
  Surface treatement for high-friction interface with human hair davidHMC 2 6,039 06-22-2009, 07:47 PM
Last Post: Gordon
  Interface separation in Copper Nickel Indium coating Donald 10 19,154 04-26-2009, 02:30 AM
Last Post: Donald
  interface oxide codep 10 15,265 03-18-2009, 06:11 AM
Last Post: codep
  Interface separation: Process or Bakelite? gejohn 2 6,836 02-05-2008, 12:18 PM
Last Post: Gordon



Users browsing this thread: 1 Guest(s)





Surface Engineering Forum Sponsor - Alphatek Hyperformance Coatings Ltd