Chromium carbide parameters for HVOF JP500
06-16-2020, 08:41 AM,
#1
Chromium carbide parameters for HVOF JP500
Dear All,
do somebody have the recomended spray parameters by Praxair for Cr3C2/NiCr 75/25?
We have a problem with low coating thickness per pass - it is only 0,015 mm.

We use this parameters:
barrel: 6"
oxygen flow: 873 slpm
kerosene flow: 0,379 slpm
feed rate: aprox. 58 g/min

Thanks for help.
Reply
06-16-2020, 01:11 PM,
#2
RE: Chromium carbide parameters for HVOF JP500
I suppose Praxair does. Why not ask them? TAFA makes JP5000 and I suppose you are buying Praxair powder. Ask your sales rep, if they don't know, tell them to find out if they want you to keep buying their powder.
Reply
07-01-2020, 04:27 PM,
#3
RE: Chromium carbide parameters for HVOF JP500
Hi Jaryn, I'm the UK sales rep for Praxair. Please feel free to send me your email address by DM if you're still experiencing issues.
Reply




Possibly Related Threads…
Thread Author Replies Views Last Post
  Praxair Ni-248 - HVOF Parameters Lars.Patrick 0 646 08-30-2023, 08:21 PM
Last Post: Lars.Patrick
Photo Pitting in HVOF Tungsten Carbide mrobie 4 3,295 08-31-2022, 02:08 PM
Last Post: Red Baron
  Epoxy Sealants for Ceramic Chromium Oxide DMan 0 1,688 06-27-2021, 11:39 AM
Last Post: DMan
  Request for solution to reduce porosity in HVOF Tungsten Carbide Coatings sreenuvundela 7 12,987 07-22-2020, 08:01 AM
Last Post: Simon Kim
  Tungsten Carbide HVOF Removal PrecisionCarbide 9 15,626 02-24-2020, 11:17 AM
Last Post: Packiaraj Mutharasu
  HVOF JK parameters for T800 plyer 8 14,639 07-27-2017, 01:41 PM
Last Post: technovel
  Cr2O3 chromium oxide spray problems by Plasma anne 9 10,137 08-01-2016, 08:15 PM
Last Post: anne
  HVOF Tungsten Carbide - New Line Setup David 1 5,263 08-16-2014, 03:51 PM
Last Post: Gordon
  Tungsten Carbide HVOF Coated Ball Valves grinding and Lapping constraints --- Reg sreenuvundela 4 11,883 07-29-2013, 09:04 AM
Last Post: Met.Eng.
  Blistering problem in Chromium Carbide Coating -- Reg sreenuvundela 4 8,178 04-28-2013, 07:14 PM
Last Post: shantanu
  Chromium Carbide crack novakmichal86 4 8,164 03-01-2013, 09:04 AM
Last Post: kschewe
Rolleyes HVOF -DJ Parameters DrTofi 2 5,921 06-19-2012, 09:25 PM
Last Post: DrTofi
  Buffer or build up layers under HVOF Carbide Coatings Stephen Booth 12 20,183 05-19-2011, 11:00 PM
Last Post: Met.Eng.
Shy Chromium Oxide Coating - Surface Finish Ra values Ian Mc 5 13,154 05-15-2009, 05:17 PM
Last Post: Gordon
  5pII chromium oxide coating ehsan 5 8,794 04-12-2009, 11:15 PM
Last Post: Gordon



Users browsing this thread: 1 Guest(s)





Surface Engineering Forum Sponsor - Alphatek Hyperformance Coatings Ltd