Hardness of Inconel 625 after ground
05-06-2018, 10:49 AM,
#1
Hardness of Inconel 625 after ground
Team,

Can anyone tell the required hardness of below material after spray and ground?
NI-328-5 / 1265F equal to Inconel 625
NiCrMoNb
(Atomized)

After ground and honed, i used to measure the diameter of the cylinder
by using bore gauge, i got few scratch marks. i feel the coating hardness is less. i have got only 25-30 HRC.

please add your comments..

Regards,
DK
Reply
05-06-2018, 12:05 PM,
#2
RE: Hardness of Inconel 625 after ground
Below Parameters i have used

Gun SG100 Praxair
Primary gas as Argon 50
Secondary gas as Helium 110
Carrier Gas as argon 35
800A
38-39 V
Spray distance 3.75"
Spray rate 4lbs/hr
Reply
05-06-2018, 12:08 PM,
#3
RE: Hardness of Inconel 625 after ground
Hi demionkrishan

You say 25-30 HRC, but what was the actual hardness test method and results?
What is the thickness of coating tested?

As a ball park figure 25-30 HRC equivalent is pretty much what to expect, though possibly a little harder depending on how it was sprayed.
Reply
05-06-2018, 12:28 PM,
#4
RE: Hardness of Inconel 625 after ground
(05-06-2018, 12:08 PM)Gordon Wrote: Hi demionkrishan

You say 25-30 HRC, but what was the actual hardness test method and results?
What is the thickness of coating tested?

As a ball park figure 25-30 HRC equivalent is pretty much what to expect, though possibly a little harder depending on how it was sprayed.


Hi Gordon,
Coating Thickness range is between 200-250 microns. I have used portable hardness tester, Rockwell C scale. it is cylindrical part so i can't get accurate reading. while i insert the piston, i found some scratch mark. so i feel my coating is smooth. May i know the Actual hardness of Inconel 625 after ground?
Reply




Possibly Related Threads…
Thread Author Replies Views Last Post
  Inconel 625 Plasma Sprayed Compressor Cylinder (ID) demionkrishan 4 2,967 06-17-2019, 01:32 PM
Last Post: demionkrishan
  Inconel 625 or NiAl 95/5 Iwan Sedaryawan CA 2 3,881 09-25-2015, 10:21 AM
Last Post: Joris Kraak
  Loading of Barrel when spraying Inconel 625 Bob Weber 11 10,006 12-31-2014, 08:52 AM
Last Post: Bob Weber
  pencil hardness and tukon hardness test transit 6 19,633 10-04-2012, 02:15 PM
Last Post: bruisjem
  F4 Gun+Tristar+muticoat+inconel 718+unmelted Bler 0 3,097 07-20-2012, 07:32 AM
Last Post: Bler
  Inconel 625 - JP5000 SDA 7 10,164 12-28-2011, 06:54 PM
Last Post: djewell
  Hardness of Inconel 625 Met.Eng. 2 12,361 08-29-2011, 09:32 AM
Last Post: Met.Eng.
  Inconel 625 coating on flange surface gops123 5 12,806 04-05-2011, 01:54 PM
Last Post: Stuart Milton



Users browsing this thread: 1 Guest(s)





Surface Engineering Forum Sponsor - Alphatek Hyperformance Coatings Ltd