In Reply to:coating on callender rolls of paper industries posted by shyam ladkani

: kindly advise me on wear ressitant coating on callender rolls .what will be most suitable alloy and equipment.these are worn out chilled iron rolls
: shyam ladkani

Consider:
HVOF tungsten carbide/cobalt chromium (86/10/4). Chromium carbide/nickel chromium and hard nickel chromium self-fluxing alloys are also used sometimes.

Arc sprayed high chromium carbon iron alloys.

Regards Gordon